TROUBLE SHOOTING IN TRIVALENT CHROME PLATING
TriCOL Decor
Problems |
Causes |
Solution |
Dark streaks |
Low TriCOL replenisher 300 |
Add slowly TriCOL replenisher 300 0.5-1 ml/l and Hull cell test |
Low specific gravity |
Adjust the tank density to standard 1.20-1.22. Adding 21 g/l of TriCOL T-Salts 100 will increase the density of the solution by 0.01 units. |
|
Metallic contamination |
Dummy 1-3 A/dm2, if the AAS analysis results show high impurity content, turn on the dummy combined ion exchanger. Note if Ni2+ is high, it is necessary to increase washing after Nickel plating and change the washing tank regularly. Repeat setting up the spray washing system before entering the Cr3+ plating bath. |
|
Organic contamination |
Carbon Treat |
|
Low TriCOL Antimist 400 |
Add slowly TriCOL Antimist 400 |
|
Poor Coverage |
Low pH |
Increase pH to standard range 2.8-3.2 |
Low specific gravity |
Adjust the tank density to standard 1.20-1.22. Adding 21 g/l of TriCOL T-Salts 100 will increase the density of the solution by 0.01 units. |
|
High temperature |
Use the cooling system to adjust the temperature to 29-320C |
|
Low TriCOL CD Plus 500 |
Add slowly TriCOL CD Plus 500 |
|
Low current density |
Adjust current density up to 10-12 A/dm2. |
|
High aeration |
Reduce aeration |
|
Patchy White Deposit |
Organic contamination |
Carbon Treat |
Dry-on of nickel plating solution |
Transfer racks faster, increase rising time, lower nickel temperature. Delay current initiation in TriCOL plating bath |
|
Contaminated nickel rinses |
Replace the nickel-plated rinse water tank, Run the ion exchange system to lower the concentration of Ni2+ ions to the allowable level. |
|
Zinc contamination |
Dummy at current density range:1-3 A/dm2 |
|
Low plating speed (less than 0.2 µm/min) |
Low current density |
Adjust current density up to 10-12 A/dm2. |
Low specific gravity |
Adjust the tank density to standard 1.20-1.22. Adding 21 g/l of TriCOL T-Salts 100 will increase the density of the solution by 0.01 units. |
|
Anodes coated |
Check anodes and clean |
|
High pH |
Adjust the pH in the range of 2.8-3.2 |
|
Low TriCOL replenisher 300 |
Add slowly TriCOL replenisher 300 0.5-1 ml/l and Hull cell test |
|
Non-Uniform Thickness |
Low aeration |
Increase agitation |
Low TriCOL Antimist 400 |
Add slowly TriCOL Antimist 400 |
|
Low TriCOL replenisher 300 |
Low: Add TriCOL replenisher 300 slowly add 0.5-1 ml/l then Hull cell test |
|
High TriCOL replenisher 300 |
High: Carbon filter then Hullcell test |
|
The anode area is not 1.5 times larger than the cathode. |
Reduce the area to be coated or increase the anode area |
|
Note: If there are errors other than the ones mentioned above, please contact the Metatech technical team. |